Soft magnetic alloy are in weak magnetic field with high permeability and low coercive force of alloys.This kind of alloy are widely used in radio electronics, precision instruments and meters, remote control and automatic control system, the combination is mainly used for energy conversion and information processing, the two aspects of is an important material in the national economy.
Introduction to the
Chemical composition
composition | C | P | S | Mn | Si |
≤ | |||||
Content(%) | 0.03 | 0.02 | 0.02 | 0.3~0.6 | 0.15~0.3 |
composition | Ni | Cr | Mo | Cu | Fe |
Content(%) | 79.0~81.0 | - | 4.8~5.2 | ≤0.2 | Bal |
Heat treatment system
shop sign | Annealing medium | heating temperature | Keep the temperature time/h | Cooling rate |
1j85 | Dry hydrogen or vacuum, pressure is not greater than 0.1 Pa | Along with the furnace heating up 1100~1150℃ | 3~6 | In 100 ~ 200 ℃ / h speed cooling to 600 ℃, fast to 300 ℃ draw a charge |
Soft magnetic alloy outer magnetic field under the action of easy
magnetization, basic disappear after removal of magnetic field of
magnetic induction intensity and magnetic alloys.
The hysteresis loop area is small and narrow, coercive force
generally below 800 a/m, high resistivity, eddy current loss is
small, high permeability, high saturation magnetic induction.Are
generally processed into sheets and strip.Melt was prepared.Mainly
used for electrical appliances, telecommunications industry in
various core components (such as transformer core, relay iron core,
choke coil, etc.).Commonly used soft magnetic alloy has a low
carbon electrical steel, eminem iron, silicon steel sheet, soft
magnetic alloy, iron, cobalt soft magnetic alloy, nickel iron iron
silicon soft magnetic alloy, etc.
Physical properties
Under the action of outside magnetic field easily after
magnetization, except to the magnetic field of magnetic induction
intensity (magnetic induction) and basic disappearance of magnetic
alloy.Hysteresis loop area is small and narrow, coercive force (Hc)
average less than 10 Oe (see precision alloy).In the late 19th
century made of low carbon steel motor and transformer core.1900
magnetic higher silicon steel sheet quickly replaced the low-carbon
steel, used in the manufacture of electric power industry
products.In 1917 the Ni - Fe alloy to adapt to the current needs of
the telephone system.Then the Fe - Co alloy with different magnetic
properties (1929), Fe - Si - Al alloy (1936) and Fe - Al alloy
(1950) to meet the special purpose.In 1953 China began production
of hot rolled silicon steel sheet.The late '50 s and began to study
Ni - Fe and soft magnetic alloy such as Fe, Co, 60 s gradually
began to produce some of the major soft magnetic alloy.In the 70 s
production of cold rolled silicon steel belt.
The magnetic properties of soft magnetic alloy mainly is: (1)
coercive force (Hc) and low hysteresis losses (Wh);(2) resistivity
(rho) is higher, low eddy current loss (We);(3) initial
permeability (mu 0) and the maximum high